Cementation Steels

Cementation process not only improves surface hardness, abrasion resistance and continuous strength, but also improves part core strength and ductility. In this way, it is ensured that large loads are carried and impact-like loads are met.

The carbon ratio of cementation materials is generally between 0.10 - 0.20%, in some varieties it can be up to 0.25%. They can be produced with or without alloys.

Cementation steels can be heat treated in different ways after the cementation process. After the cementation process, the carbon content in the core region remains at 0.10 - 0.20%, while the carbon content in the surface region increases up to 0.8%. In this case, the selection of the heat treatment temperature to be made becomes difficult due to the varying amount of carbon in each part of the part structure. The temperature to be selected based on the core region causes grain coarsening in the part wall region, and the temperature to be selected based on the part wall region causes the core region to not harden sufficiently. For this reason, the easiest method to be applied is direct hardening from the cementation temperature. This method can only be applied after salt bath and gas cementation. The method is more suitable for fine-grained steels.

Core strength can be increased with the increase of carbon content and added alloying elements in cementation steels. However, the most efficient result can be achieved with core hardening after cementation. This method is called double hardening. The part, which is abruptly cooled from the appropriate hardening temperature in the core region, is subjected to the intermediate annealing process, and then the hardness of the wall region is provided by sudden cooling from the hardening temperature suitable for the wall region.

Welding capabilities of cementation steels are good. Alloy steels require annealing after welding. Machining is best achieved with normally annealed or coarse-grained material. The softened material is not preferred because it gives bad surface quality.

CEMENTATION STEELS AND COMPOSITIONS
material no. RELIGION SAE / AISI NS NS mn Pmax Smax cr B.C Ni
1.0301 C 10 1010 0.07-0.13 0.04 0.30-0.60 0.045 0.045 – – –
1.0401 C 15 1015 0.12-0.18 0.04 0.30-0.80 0.045 0.045 – – –
1.1121 Ck 10 1010 0.07-0.13 0.04 0.30-0.60 0.035 0.035 – – –
1.1141 Ck 15 1015 0.12-0.18 0.04 0.30-0.60 0.035 0.035 – – –
1.7015 15 Cr 3 5015 0.12-0.18 0.15-0.40 0.40-0.60 0.035 0.035 0.40-0.70 – –
1.7131 16 MnCr 5 5115 0.14-0.19 0.04 1.00-1.30 0.035 0.035 0.80-1.10 – –
1.7147 20 MnCr 5 5120 0.17-0.22 0.04 0.60-0.90 0.035 0.035 1.00-1.30 – –
1.7321 20 MoCr 4 – 0.17-0.23 0.04 0.70-1.00 0.035 0.035 0.30-0.60 0.40-0.50 –
1.7325 25 MoCr 4 – 0.23-0.29 0.15-0.40 0.60-0.90 0.035 0.035 0.40-0.60 0.40-0.50 –
1.5919 15 CrNi 6 – 0.14-0.19 0.04 0.40-0.60 0.035 0.035 1.40-1.70 – 1.40-1.70
1.5920 18 CrNi 8 – 0.15-0.20 0.15-0.40 0.40-0.60 0.035 0.035 1.80-2.10 – 1.80-2.10
1.6587 17 NiCrMo 6 – 0.14-0.21 0.04 0.50-0.90 0.035 0.035 1.50-1.80 0.25-0.35 1.40-1.70
1.6523 21 NiCrMo 2 8620 0.17-0.23 0.04 0.65-0.95 0.035 0.040 0.35-0.70 0.15-0.25 0.40-0.70
1.1140 cm 15 – 0.12-0.18 0.04 0.30-0.60 0.035 0.020-0.040 – – –
1.7139 16 MnCrS 5 – 0.14-0.19 0.04 1.00-1.30 0.035 0.020-0.040 0.80-1.10 – –
1.7149 20 MnCrS 5 – 0.17-0.22 0.04 1.10-1.40 0.035 0.020-0.040 1.00-1.30 – –
1.7323 20 MoCrS 4 – 0.17-0.22 0.04 0.60-0.90 0.035 0.020-0.040 0.30-0.50 0.40-0.50 –
1.7326 25 MoCrS 4 – 0.23-0.29 0.15-0.40 0.60-0.90 0.035 0.020-0.040 0.40-0.60 0.40-0.50 –
1.5713 13 NiCr 6 3415 0.10-0.17 0.15-0.35 0.30-0.50 0.035 0.035 0.65-0.85 – 1.35-1.50
1.5752 14 NiCr 14 3415;3310 0.14-0.20 0.04 0.40-0.70 0.035 0.035 0.60-0.90 – 3.00-3.50
1.7243 18CrMo 4 – 0.15-0.21 0.04 0.60-0.90 0.035 0.035 0.90-1.20 0.15-0.25 –

JOMINY VALUE
HRC values from the instantly cooled surface ( mm )
QUALITY 1.5 3 5 7 9 11th 13 15 20 25 30 35 40
15 CrNi 6 Max 47 47 46 45 43 42 41 39 37 35 34 34 33
21 NiCrMo 2 Max 49 48 44 42 36 32 30 29 26 24 23 23 22
17 NiCrMo 6 Max 48 48 48 48 47 47 46 46 44 43 42 41 41
16 MnCr 5 Max 47 46 44 41 37 35 34 33 31 30 29 28 27
20 MnCr 5 Max 49 49 48 46 44 42 41 40 37 35 34 33 31
20 MoCr 4 Max 49 47 43 40 36 34 31 29 26 24 23 22 21
25 MoCr 4 Max 52 51 50 47 43 40 38 36 33 31 30 29 28

CEMENTATION STEELS
material no. RELIGION SAE / AISI USAGE PLACES
1.0301 C 10 1010 Low core strength and medium stress structural and machine parts
1.0401 C 15 1015 Lever arms, bushings, pulleys, gear wheels, measuring instruments and similar structural and machine parts
1.1121 Ck 10 1010 White furniture and office machine wear parts such as low core strength lever arm, bushing, pin
1.1140 cm 15 – Vibrating and low core stress structures and machine parts
1.1141 Ck 15 1015 Small machine parts such as low core strength lever arm, bushing, pin journal
1.5713 13 NiCr 6 3415 Small-sized, over-stressed parts such as gear wheels, sprockets, shafts in machinery and automobiles
1.5752 14 NiCr 14 3415;3310 Camshafts, gear wheel, standard tension universal joints
1.5919 15 CrNi 6 – Small-sized, over-stressed parts such as gear wheels, sprockets, shafts in machinery and automobiles
1.5920 18 CrNi 8 – High-stress driveline parts such as thick-section gear wheels, plate gears, and drive parts
1.6523 21 NiCrMo 2 8620 Gear wheels, pins, shafts, switch sleeves and similar parts in machines and automobiles that are under high stress.
1.6587 17 NiCrMo 6 – Highly stressed parts of the drivetrain, thick-section impellers, similar wear parts
1.7015 15 Cr 3 5015 Roller bearing, pulley, gauge, piston pin, differential part, gear wheel, ball screw, etc.
1.7131 16 MnCr 5 5115 Gear wheel, driveline parts, cardan socket, shaft, pin, bushing and similar parts
1.7139 16 MnCrS 5 – 1.7131 materials with improved machining properties by adding sulfur
1.7147 20 MnCr 5 5120 Driveline parts, gear wheels, plates and bevel gears, thick-section shafts, pins, bushings and similar parts
1.7149 20 MnCrS 5 – 1.7147 materials with improved machining properties by adding sulfur
1.7243 18CrMo 4 – All kinds of drivetrain, steering parts, axles, shafts, pins, bushings, switchgear bearing parts
1.7321 20 MoCr 4 – All kinds of drivetrain, steering parts, axles, shafts, pins, bushings, switchgear bearing parts
1.7323 20 MoCrS 4 – All kinds of drivetrain, steering parts, axles, shafts, pins, bushings, switchgear bearing parts
1.7325 25 MoCr 4 – All kinds of drivetrain, steering parts, axles, shafts, pins, bushings, switchgear bearing parts
1.7326 25 MoCrS 4 – All kinds of drivetrain, steering parts, axles, shafts, pins, bushings, switchgear bearing parts
HEAT TREATMENT OF CEMENTATION STEELS
material no. RELIGION SAE / AISI Hot Figure. Temperature ( °C ) Soft Annealing Temperature ( °C ) Cementation Temperature ( °C ) Cementation Post-cementation cooling Core Hardening Temperature Intermediate Annealing Temperature Wall Hardening Tempering Temperature
Operation Style That oil hot bath salt bath sem. Box weather ( °C ) That oil hot bath
Direct S. Simple S. Double S.
1.0301 C 10 1010 1150-850 670-700 900-950 * * – * – * – * * 880-920 – – – – – 150-180
1.0401 C 15 1015 1150-850 670-700 900-950 * * – * – * – * * 880-920 – – – – – 150-180
1.1121 Ck 10 1010 1150-850 670-700 900-950 * * – * – * – * * 880-920 – – – – – 150-180
1.1140 cm 15 – 1150-850 670-700 900-950 * * – * – * – * * 880-920 – – – – – 150-180
1.1141 Ck 15 1015 1150-850 670-700 900-950 * * – * – * – * * 880-920 – – – – – 150-180
1.5919 15 CrNi 6 – 1150-850 670-700 900-950 – * * – * * * * * 840-870 630-650 800-830 + * * 170-210
1.5920 18 CrNi 8 – 1150-850 670-700 900-950 – * * – * * * * * 840-870 630-650 800-830 + * * 170-210
1.6523 21 NiCrMo 2 8620 1150-850 670-700 900-950 * * – – * * – * * 840-870 630-650 800-830 + * * 170-210
1.6587 17 NiCrMo 6 – 1150-850 670-700 900-950 – * * – * * * * * 840-870 630-650 800-830 + * * 170-210
1.7015 15 Cr 3 5015 1150-850 670-700 900-950 * * – * * * – * * 870-900 – – – – – 150-180
1.7131 16 MnCr 5 5115 1150-850 670-700 900-950 + * * – * * * * * 850-880 – 810-840 + * * 170-210
1.7139 16 MnCrS 5 – 1150-850 670-700 900-950 + * * – * * * * * 850-880 – 810-840 + * * 170-210
1.7147 20 MnCr 5 5120 1150-850 670-700 900-950 + * * – * * * * * 850-880 – 810-840 + * * 170-210
1.7149 20 MnCrS 5 – 1150-850 670-700 900-950 + * * – * * * * * 850-880 – 810-840 + * * 170-210
1.7321 20 MoCr 4 – 1150-850 670-700 900-950 * – – – * * – – – 890-920 – – – – – 170-210
1.7323 20 MoCrS 4 – 1150-850 670-700 900-950 * – – – * * – – – 890-920 – – – – – 170-210
1.7325 25 MoCr 4 – 1150-850 670-700 900-950 * – – – * * – – – 890-920 – – – – – 170-210
1.7326 25 MoCrS 4 – 1150-850 670-700 900-950 * – – – * * – – – 890-920 – – – – – 170-210
* priority preferred + second preferred – not applicable